Comparison table
| Grade | Chemistry / cell | Density | CFD @ 25% | Continuous temp. | Fire / compliance | Raw sheet $/ft² |
|---|---|---|---|---|---|---|
| PORON® 4701-30 | Microcellular PU | ~15 lb/ft³ (240 kg/m³) | 2–4 psi (14–28 kPa) | −51 to +90°C | FMVSS 302; UL 94 HBF/HF-1 grades | $2.50–$6.00 (1/16"–1/8") |
| PORON® 4701-40 | Microcellular PU | ~15 lb/ft³ (240 kg/m³) | 4–11 psi (27–76 kPa) | −51 to +90°C | FMVSS 302; 40V0 UL 94 V-0 | $2.50–$5.50 (1/16") |
| PORON® 4701-50 | Microcellular PU | ~30 lb/ft³ (480 kg/m³) | 15–45 psi (103–310 kPa) | −51 to +90°C | FMVSS 302 | $3.50–$7.00 (1/16") |
| BISCO® HT-800 | Closed-cell silicone | ~22 lb/ft³ (352 kg/m³) | 6–14 psi (typ. 9.7) | −55 to +200°C | UL 94 V-0, HF-1; ASTM E162/E662; FDA 177.2600 | $4.00–$9.00 (1/16"–1/8") |
| Plastazote® LD45 | Closed-cell XLPE (N₂) | 2.8 lb/ft³ (45 kg/m³) | ~13.6 psi (94 kPa) | −70 to +105°C | FR grades: FMVSS 302, FAR 25.853 | $0.75–$2.50 (1/4"–1/2") |
| Basotect® G+ / UL | Open-cell melamine | 0.56 lb/ft³ (9 kg/m³) | >1.0 psi (>7 kPa) | −200 to +240°C | UL 94 V-0, HF-1; FMVSS 302; FAR 25.853 (UL) | $1.50–$3.50 (1") |
| ASTM D1056 2A1 EPDM | Closed-cell sponge | ~7–10 lb/ft³ | 2–5 psi | −40 to +105°C | Weather / UV / ozone | $0.85–$2.20 (1/8"–1/4") |
| ASTM D1056 2A2 EPDM | Closed-cell sponge | ~8–12 lb/ft³ | 5–9 psi | −40 to +105°C | Outdoor HVAC / enclosure seal | $0.95–$2.50 (1/8"–1/4") |
| ASTM D1056 2A3 EPDM | Closed-cell sponge | ~10–14 lb/ft³ | 9–13 psi | −40 to +105°C | High bolt-load seals | $1.10–$2.80 (1/8"–1/4") |
| ASTM D1056 2C2 neoprene | Closed-cell CR blend | ~10–14 lb/ft³ | 5–9 psi | −40 to +93°C | Medium oil; UL 94 HF-1 grades | $1.20–$3.00 (1/8"–1/4") |
| ESD conductive XLPE / PU | Carbon-loaded PE or PU | 2.0–4.0 lb/ft³ | 6–14 psi (PE) / 0.5–2 (PU) | −40 to +90°C | ANSI/ESD S20.20, S541 | $1.80–$4.80 (1/4"–1") |
| PU ester / ether, 2 lb | Open-cell flexible PU | 1.8–2.2 lb/ft³ | 0.4–1.2 psi (ILD 25–45) | −40 to +95°C | MIL-PRF-26514 cushioning | $0.40–$1.40 (1/2"–2") |
How to read the numbers
CFD @ 25% (compression force deflection)
The pressure needed to compress the foam to 75% of its thickness. It sets the closure force a gasket needs and is the basis of the ASTM D1056 grade number. Double the contact area and the force doubles; go from 25% to 50% deflection and the force rises roughly 2.65 times. Size it in the gasket force calculator.
Open-cell vs closed-cell
Closed-cell foams (EPDM and neoprene sponge, XLPE, cellular silicone) do not wick water and seal against immersion. Open-cell foams (melamine, flexible PU) breathe and absorb sound. Microcellular PORON® sits between: very fine cells that seal dust and splash and recover almost completely, but it is not the choice for continuous immersion.
Continuous temperature
The temperature the material tolerates for its service life, not the short excursion limit. PORON® is rated 90°C continuous (121°C intermittent); move to BISCO® silicone for 200°C or melamine for 240°C.
Compression set
The share of deflection the foam does not recover after being held compressed. Low compression set (under 5% for PORON® 4701) keeps a gasket sealing for years; high compression set means it relaxes and leaks.
Material deep-dives
PORON® vs BISCO® HT-800
Urethane vs silicone for EV, electronics and enclosure gaskets.
Read the comparisonBasotect® melamine & ESD foams
Acoustic absorbers and electrostatic-safe electronics foams.
Read the guide