Three ways to die cut foam
Flatbed steel-rule
A hardened steel rule bent to the part outline and set in a die board. The workhorse for gaskets, pads and through-cut parts from sheet. Lowest tooling cost; die boards are cheap to remake when the drawing changes.
Rotary die
A machined or flexible magnetic die on a cylinder, fed from roll stock. Highest speed and tightest registration for thin PORON® and PSA parts in very high volume.
Kiss-cutting
The rule cuts through the foam and adhesive but stops at the liner, so parts stay on a carrier sheet or roll for peel-and-place assembly. Needs depth control within a few thousandths.

Tooling cost tiers
| Die type | Indicative tooling | What drives the cost |
|---|---|---|
| Simple 2D through-cut (pad, rectangle, ring) | $300–$500 | Rule length, one cavity |
| Intricate 2D gasket with bolt holes and cutouts | $800–$1,200 | Internal punches, ejection rubber, narrow webs |
| Kiss-cut on liner / multi-cavity | $1,500–$2,500+ | Depth control, multiple cavities, liner tabs, rotary tooling |
Press setup on top of tooling typically runs around $125 per job. After that the cut itself costs only a few cents per part, which is why die cutting wins at volume. The break-even against waterjet is:
Break-even qty = (Die tooling + Die setup − Waterjet setup) ÷ (Waterjet cost per part − Die cost per part)
Material cost cancels out of the equation because both processes cut the same nested sheet. Run it for your part in the conversion cost estimator.
Design for die cutting
- Minimum web width: keep material between cutouts at least equal to the foam thickness, and never under about 1/16" (1.6 mm) on soft foams; thin webs tear on ejection.
- Hole-to-edge distance: at least 1.5× the thickness, or the hole will distort the outer edge.
- Small holes: holes smaller than the material thickness do not eject cleanly from a steel-rule die; specify punches or move them to waterjet.
- Corner radii: sharp inside corners on a steel rule need relief cuts; a 1/32" radius cuts cleaner and lasts longer.
- Thickness: foam over about 1" compresses under the rule and leaves a concave (dished) edge. Use waterjet or CNC for thick parts.
- Liner tabs: on kiss-cut parts, add a lift tab or an extended liner so assemblers can start the peel.
Low-surface-energy foams: kiss-cut Plastazote®, ESD XLPE, EPDM and BISCO® need a PSA matched to the substrate (3M 9474LE or a silicone dual-liner). A 200MP acrylic will pass a peel test on day one and lift in the field. See PSA lamination.
Tolerances you can expect
A standard steel-rule die holds ARPM BL2 (±0.032" under 1", ±0.040" from 1" to 6.3"). A tight die with machined rule and controlled ejection holds ±0.010"–±0.030" on stable materials such as PORON® and BISCO®. Very soft open-cell foams relax after cutting and are better specified to BL2 or BL3.